Carefully observed decisions and firing instructions for creating with glass. Thoughts on color, placement and reactions achieved through the glass work.
Friday, May 2, 2014
Contour Fuse firing schedule
This worked nicely for a 6mm 2 layers of clear glass with premade fused flowers on top along with stringers and chunky mixed color frit along with fine grit. The schedule I used is as follows:
300 dph...............................................1150 degrees................................hold 20 mins
Full......................................................1425 degrees................................hold 12 mins
Full........................................................900 degrees................................hold 1 hour
150 dph.................................................800 degrees.................................hold 2 mins
Off
Three of the four corners fused fully. One of the corns appears uneven, like the top layer was a little short of the bottom and it did not quite meet it. But not bad all in all. I had originally intended to slump it but now I think it would be better to keep it as a tile.
Contour is between tack fusing and full fusing, a nice mixture not a precisely defined, bumpy surface but not flat and loosing all its surface texture.
300 dph...............................................1150 degrees................................hold 20 mins
Full......................................................1425 degrees................................hold 12 mins
Full........................................................900 degrees................................hold 1 hour
150 dph.................................................800 degrees.................................hold 2 mins
Off
Three of the four corners fused fully. One of the corns appears uneven, like the top layer was a little short of the bottom and it did not quite meet it. But not bad all in all. I had originally intended to slump it but now I think it would be better to keep it as a tile.
Contour is between tack fusing and full fusing, a nice mixture not a precisely defined, bumpy surface but not flat and loosing all its surface texture.